Method of manufacturing surgical implants from cast stainless steel and product
Assignee: Smith and Nephew Inc
•
Filing: 1986-04-03
•
Granted: 1988-10-04
•
Expires: 2006-04-03
Abstract
Abstract A surgical implant is disclosed manufactured from cast austenitic stainless steel and cold-forged to a final shape. The endoprosthesis is initially a preform which is cast oversized in shape and dimensions. It is then compressed using the cold-forging process to its final size and shape. Using a cast material as a starting material and then compressing it substantially reduces the porosity of the material and increases its strength compared to a machined product from a wrought material.
Inventors
- 👤 John Murley
- 👤 Bob Wigginton
- 👤 Imogene Baswell
Bibliographic Details
Application Number
—
Jurisdiction
US
Data Source
google_patents
Last Synchronized
2026-10-29 09:32
CPC Classifications
C; C21; C21D; C21D8/00; B; B21; B21J; B21J5/00; B21J5/002; C21D7/00; C21D7/02; Y; Y10; Y10T; Y10T29/00; Y10T29/49; Y10T29/4998; Y10T29/49988
Claims Analysis
Total Claims: 23
Claim 1
Independent Claim
80 words
A medical prosthesis formed as a result of a method comprising the steps of: casting an oversized preform substantially in the same configuration of the medical prosthesis to be formed, from a corrosion resistant, austenitic, stainless steel; and cold-forging the preform in a closed die having cavities that correspond in shape to but are smaller than the preform, to reduce the overall dimensions of the preform to a final finished size defined by the cavity, and to strengthen the preform.
Claim 2
Dependent Claim
80 words
A medical prosthesis formed as a result of a method comprising the steps of: casting an oversized preform substantially in the same configuration of the medical prosthesis to be formed, from a corrosion resistant, austenitic, stainless steel; and cold-forging the preform in a closed die having cavities that correspond in shape to but are smaller than the preform, to reduce the overall dimensions of the preform to a final finished size defined by the cavity, and to strengthen the preform.
Claim 3
Dependent Claim
31 words
The medical prosthesis of claim 1 wherein said preform is cast with at least a portion of said preform being between about 20 and 30 percent larger than its final size.
Claim 4
Dependent Claim
27 words
The medical prosthesis of claim 2 wherein the remaining portion of said preform as cast being between about 10 and 20 percent larger than its final size.
Claim 5
Dependent Claim
18 words
The medical prosthesis of claim 1 wherein said cold-forging step comprises compressing said preform at least one time.
Claim 6
Dependent Claim
18 words
The medical prosthesis of claim 4 wherein said cold-forging step comprises compressing said preform at least three times.
Claim 7
Dependent Claim
50 words
The medical prosthesis of claim 1 further comprising the step of stress relieving the preform wherein the stress relieving step includes: heating the preform to a temperature of about 750° F. (399° C.); and maintaining the preform at said temperature for aout two hours, followed by cooling to room temperature.
Claim 8
Dependent Claim
25 words
The medical prosthesis of claim 1 further comprising the step of solution annealing the preform following said casting step but prior to said cold-forging step.
Claim 9
Dependent Claim
43 words
The medical prosthesis of claim 7 wherein said solution annealing step comprises: heating the preform to a temperature of about 2000° F. (1093° C.); and maintaining the preform at said temperature for at least one-half hour, followed by rapid cooling to room temperature.
Claim 10
Dependent Claim
14 words
The medical prosthesis of claim 1 wherein said medical prosthesis is a hip prosthesis.
Claim 11
Dependent Claim
18 words
The medical prosthesis of claim 9 wherein said corrosion resistant austenitic stainless steel is Type 316L stainless steel.
Claim 12
Dependent Claim
23 words
The medical prosthesis of claim 10 wherein said cold-forging step includes applying a force between about 500 metric tons and 525 metric tons.
Claim 13
Independent Claim
42 words
A method of manufacturing a medical prosthesis comprising the step of: casting an oversized preform from austenitic stainless steel; and cold-forging the preform in closed dies to reduce the overall dimension of the preform to finished size and to strengthen the preform.
Claim 14
Independent Claim
42 words
A method of manufacturing a medical prosthesis comprising the step of: casting an oversized preform from austenitic stainless steel; and cold-forging the preform in closed dies to reduce the overall dimension of the preform to finished size and to strengthen the preform.
Claim 15
Dependent Claim
49 words
The method of claim 12 further comprising the step of stress relieving the preform wherein the stress relieving step includes: heating the preform to a temperature of about 750° F. (399° C.); and maintaining the preform at said temperature for about two hours, followed by cooling to room temperature.
Claim 16
Dependent Claim
24 words
The method of claim 12 further comprising the step of solution annealing the preform following said casting step but prior to said cold-forging step.
Claim 17
Dependent Claim
42 words
The method of claim 14 wherein said solution annealing step comprises: heating the preform to a temperature of about 2000° F. (1093° C.); and maintaining the preform at said temperature for at least one-half hour, followed by rapid cooling to room temperature.
Claim 18
Dependent Claim
13 words
The method of claim 12 wherein said medical prosthesis is a hip prosthesis.
Claim 19
Dependent Claim
17 words
The method of claim 16 wherein said corrosion resistant austenitic stainless steel is Type 316L stainless steel.
Claim 20
Dependent Claim
17 words
The method of claim 12 wherein said cold-forging step comprises compressing said preform at least one time.
Claim 21
Dependent Claim
17 words
The method of claim 18 wherein said cold-forging step comprises compressing said preform at least three times.
Claim 22
Dependent Claim
30 words
The method of claim 12 wherein said preform is cast with at least a portion of said preform being between about 20 and 30 percent larger than its final size.
Claim 23
Dependent Claim
26 words
The method of claim 20 wherein the remaining portion of said perform as cast being between about 10 and 20 percent larger than its final size.
References Cited (Backward Citations)
US2358799A
Cited
US2871557A
Cited
US3197997A
Cited
US3284250A
Cited
US3340048A
Cited
US3399560A
Cited
US3645124A
Cited
US3737981A
Cited
US3821843A
Cited
US3740274A
Cited
US3871925A
Cited
US4253323A
Cited
USPTO Annuity & Maintenance Windows
| Annuity Stage | Window Opens | Payment Deadline | Surcharge Period Until | Estimated Fee | Status |
|---|---|---|---|---|---|
| 3.5 Years (Year 4) | 1991-10-04 | 1992-04-04 | 1992-10-04 | $2000.00 | Window Closed / Lapsed |
| 7.5 Years (Year 8) | 1995-10-04 | 1996-04-04 | 1996-10-04 | $3760.00 | Window Closed / Lapsed |
| 11.5 Years (Year 12) | 1999-10-04 | 2000-04-04 | 2000-10-04 | $7700.00 | Window Closed / Lapsed |